Steel doesn't care that it's January, but the weld does. Here is what changes when the metal is far below freezing.
Equipment parked outside in the Red River Valley sits at whatever temperature the night was. In the cold snap at the end of January 2019, the National Weather Service in Grand Forks logged -35°F at the airport on January 30 and -32°F the next day, breaking the old January 31 record of -29°F set in 1996. Wind chills reached -61°F. A frame rail or loader arm that spent the night in that is the base metal a welder starts with.
Lincoln Electric lists four main reasons to preheat before welding:
Lincoln names ambient temperature as one of the factors in deciding whether to preheat, alongside code requirements, thickness, steel chemistry, restraint, the hydrogen level of the filler metal, and any history of cracking. It also says that without a code, preheat usually isn't required on low-carbon steel under 1 inch thick, and that the need rises as chemistry, hydrogen, restraint and thickness go up. Miller notes that operations commonly preheat steel 1 inch thick or more.
When a welding code governs the work (structural steel, for example), the code sets the minimum preheat for the steel, process and thickness, and that minimum has to be met.
Lincoln describes the AWS D1.1 structural code requirement: the minimum preheat temperature has to be reached for a distance at least equal to the thickness of the thickest part, and never less than 3 inches, in every direction from the weld. The recommended practice is to heat from the side opposite the weld, measure the surface temperature next to the joint, and check it again just before each pass. For ordinary carbon steels, Lincoln says overshooting the minimum by about 100°F is acceptable; quenched and tempered steels need both a minimum and a maximum.
Miller lists the tools welders use to check: temperature-indicating crayons, thermocouples, infrared thermometers and thermal cameras. For heating, Miller lists induction, open flame, and electric resistance pads. It notes flame preheating can heat unevenly and needs a fire watch, which matters in a shed full of straw (see our hot work guide).
TWI, the UK welding research institute, explains that hydrogen cracking needs three things at once: hydrogen from the welding process, a hard, crack-prone structure in the steel, and tensile stress. Cold steel cools a weld faster, which helps form that hard structure and gives hydrogen less time to escape.
Two TWI points matter for field repairs:
Low-hydrogen stick electrodes like E7018 only stay low-hydrogen if they stay dry. Lincoln says opened containers should be stored in a cabinet at 250–300°F, and that moisture picked up by the coating can cause porosity and, in higher-strength steels, hydrogen cracking. Its redrying table gives 650–750°F for one hour for E7018 rods exposed to air for less than a week. Rods from the "fast freeze" group (E6010 and E6011) are a different case: Lincoln does not recommend re-baking them.
Miller's storage range for E7018 is the same 250–300°F, and it describes E7018 welds as having high impact properties even in cold weather, which is one reason it is the usual rod for structural and cold-service repairs. In practice, that is why a mobile rig in winter carries a rod oven, and why a box of 7018 that sat open in the truck for a month is a problem.
Cold slows a job down. Wind can ruin it. Lincoln notes that a light breeze can wash away MIG shielding gas and cause porosity, while self-shielded flux-cored wire can withstand a strong breeze. Miller says the same about stick and flux-core in windy conditions. On a February day on open ground, a welder will often choose stick or flux-core for that reason alone, and a tarp, a trailer parked upwind, or the lee side of a building makes the work faster and better.
Cast iron is sensitive to fast cooling at any time of year, and a frozen casting pulls heat out of a weld fast. Lincoln's guidance is to either preheat the whole casting slowly or keep it at about 100°F, never so hot you can't hold your bare hand on it, and never to speed up cooling with water or compressed air. Our farm repair guide covers both methods.
Checked October 2026.
This is a referral line, not a welder. You reach the site owner, who passes your job to an independent local welder. Free to you; the welder may pay a referral fee.